Skip to content
Titanium CNC
Get a quote

Guides / Process

Machining Titanium Castings: How Much Stock to Leave, What HIP Fixes and What It Does Not

Molten metal poured into a ceramic shell mold with flame at the pouring cup, the investment casting step before titanium casting machining
Photo: 5oclockhustle, CC BY-SA 4.0, via Wikimedia Commons. The pour shown is molten steel in a ceramic shell, used to show the shell-mold process; titanium is melted and poured under vacuum.

Machine a titanium casting by planning the cut around its skin. Every investment casting leaves a hard, brittle surface layer called alpha case, and the stock you leave on a machined face has to be deeper than that layer. Inside the casting, hot isostatic pressing (HIP) can close most pores, but not all of them, and it does not make a casting behave like bar in fatigue. This guide covers how much layer to expect, what HIP fixes, which defects remain and what to write on the drawing before a shop quotes the machining.

Why a casting has a skin that bar does not

Titanium is reactive at casting temperature. It attacks most mold materials, picks up interstitial oxygen and dissolves some refractory metal from the shell. The oxygen forms alpha case, and a hardness gradient runs from the surface into the metal. A 2015 paper in the Journal of Materials Engineering and Performance notes that the gradient is not visible in the microstructure, so it is measured with microhardness traverses. It also notes that mold temperature has to stay as low as possible to limit the reaction.

Foundries fight this with zirconia or yttria face coats, because those oxides are more stable against liquid titanium. A conference paper from Akrapovic and the University of Modena says the coats help, cost more and do not remove the layer completely. The same paper gives a normal range for standard titanium castings of 50 to 500 microns, and notes that the layer deepens as the wall gets thicker and the metal stays liquid longer.

Alpha case matters to a machinist for three reasons:

  • It is harder than the metal below it, so the first cut on an as-cast face meets an abrasive skin. The paper says alpha case makes castings difficult to machine.
  • It promotes crack initiation and reduces fatigue properties, so a face left with any of it on a loaded part is a risk.
  • It is not uniform. The depth changes with wall thickness and cooling, so one part can carry several different depths.

How much stock to leave

Public data gives an order of magnitude, not a design allowance. In the Akrapovic trial, zirconia-shell test steps from 2 to 8 mm thick carried an alpha case of about 0.3 to 0.4 mm. The authors judged that an average removal of 0.35 mm, plus or minus 0.02 mm, was enough to eliminate it on both Ti-6Al-4V and commercially pure Grade 2.

Source What it reports How to use it
Akrapovic and Modena paper (2012) 0.3 to 0.4 mm alpha case on zirconia-shell steps 2 to 8 mm thick; 0.35 mm removal judged enough Sanity check on a quote, not a design value
Same paper, general range 50 to 500 microns for standard titanium castings Shows how much the process changes the number
Foundry’s own case-depth data Measured on your shell system, your wall thickness and your alloy The number the drawing allowance should be built on

So ask the foundry for its measured case depth on sections like yours, and put the machining allowance on the casting drawing with the casting tolerance added on top. Do not copy 0.35 mm from a paper. It came from one shell system in one lab.

Three consequences for the shop:

  1. A thin allowance can leave alpha case behind. A face that cleans up at one corner and not at another is the typical sign.
  2. A thick allowance costs run time. Titanium cycles are slow, so each extra tenth of a millimetre on large faces adds to the quote. See titanium machining cost.
  3. Datums need thought. If the datum faces carry the most casting variation, the first operation has to establish them. Our tolerances guide covers what to put on a drawing.

Chemical milling or machining to clear the skin

Both routes are used, and the specification for the part should name which one applies. In the Akrapovic trial, commercial pickling baths cleared a 0.3 to 0.4 mm layer in 30 to 40 minutes. Four things from that paper are worth knowing:

  • Pure titanium etched 10 to 15% faster than Ti-6Al-4V.
  • Every bath removed more metal where the wall was thicker, which the authors flag for castings with narrow tolerances.
  • Dissolved titanium in the bath has to stay below about 6 to 7 g per litre for stable results.
  • Hydrogen pickup needs control. The authors found even short cycles could approach the upper limit of 150 ppm that they cite from ASTM B367, and baths containing sulphate tended to raise hydrogen more.

Our guide to pickling and chemical milling goes through the process steps and the hydrogen check, and the welding and alpha case guide covers the same layer from the welding side.

What HIP closes and what it does not

HIP puts the casting under inert gas pressure at high temperature, so internal pores collapse and bond. A micro-CT study by researchers at Stellenbosch University and the CSIR scanned six cast Ti-6Al-4V rods before and after HIP. The authors ran six different cycles, from 100 to 170 MPa, 930 to 1050 °C and 1.5 to 4 hours, and quote 920 °C at 100 MPa for about 2 hours as the standard cycle for titanium castings. Average porosity fell from about 0.06 to 0.08% to nearly zero, and the largest pore, 2.7 mm across, closed completely.

Two limits apply:

  • Open pores stay open. HIP closes internal pores only. The paper’s introduction states that pores connected to the surface remain.
  • A few small pores can survive near the skin. Two of the six rods kept pores of 91 to 259 microns, whose nearest edges sat 30 to 64 microns below the surface. The authors suggest alpha case microcracks may connect those pores to the surface, which would stop HIP from closing them. Both rods came from the cycle with the shortest hold and fastest cooling, so cycle parameters matter.

Those surviving pores sat inside the alpha case. A machining allowance deeper than the layer therefore removes them, which is our inference from the paper’s numbers, not something the authors state. It is another reason to keep the allowance generous on faces that matter.

HIP and fatigue are a separate question. A US Bureau of Mines report (Report of Investigations 8897, 1984) found that HIP healed internal porosity in Ti-6Al-4V castings but did not significantly improve fatigue strength, and that both cast and cast plus HIP fatigue properties were significantly lower than wrought. A 2010 AeroMat paper from the PPRIME Institute and Airbus notes that surface defects such as pin holes and HIP sinks remain a concern after HIP. So HIP is a porosity tool, not a route to bar properties. If the part sees cyclic load, ask the foundry for fatigue test data on its process, or choose another route. Our forging versus bar stock guide and the 3D printed versus machined comparison set out the alternatives.

Need a quote for this part? Get a titanium quote

What to put on the drawing and the RFQ

A casting RFQ that reads like a bar RFQ gets quotes that fail on the first part. Put these items on it:

Item What to state
Casting specification The standard or customer spec the casting meets, and the grade
Machined faces Which faces are machined, with the stock allowance shown on the casting drawing
Alpha case Removal method (chemical milling or machining) and who does it
HIP Required or not, and whether the record ships with the certificate
Sequence Order of HIP, alpha case removal and final machining, written down
Inspection Radiography and fluorescent penetrant method and acceptance class. See FPI on titanium
Repair Whether weld repair is allowed and what heat treatment follows
Hydrogen Limit and the point at which it is checked after any acid process
Certificates Chemistry, heat or lot traceability and process records. See mill certificates

ASTM B367, the specification for titanium and titanium alloy castings for general corrosion-resistant and industrial use, is the usual starting point. Its summary says castings are supplied as-cast unless post-weld stress relief is required, and that they must be free of adhering mold material, scale, cracks and hot tears on visual inspection. It does not say how much stock you need for machining or what your fatigue rating is. Those come from your drawing and your foundry.

Cast or cut from bar

Casting wins when the part has complex shape, deep internal passages or a large buy-to-fly waste in bar form. It loses when the part is simple or fatigue loaded, and when the quantity is too small to carry the pattern and shell tooling. Do the arithmetic with the buy to fly calculator before you start on a casting route, and ask the shop to quote the machining separately from the casting so you can compare.

If you have a casting drawing and want shops that machine titanium castings to quote the finish work, send it through the RFQ form. We reply within 24 business hours with one itemised quote. Say whether the casting is supplied by you or has to be sourced, and say what the drawing requires for alpha case and HIP.

Sources

Frequently asked questions

Why do titanium castings need extra stock on machined faces?

Molten titanium reacts with the ceramic shell and picks up oxygen, which leaves a hard, brittle skin called alpha case. A published lab study measured about 0.3 to 0.4 mm of it on zirconia-shell castings and judged 0.35 mm of removal enough. The foundry has to leave more stock than its own case depth, then the shop cuts through it.

Does hot isostatic pressing remove all porosity from a titanium casting?

No. HIP closes internal pores, and in one micro-CT study it cut average porosity from about 0.06 to 0.08% to nearly zero. Pores connected to the surface stay open, and that study found a few small pores, 91 to 259 microns across, just under the skin of two rods. Ask for the HIP record and an inspection method.

Is a cast titanium part as strong in fatigue as one machined from bar?

Not by default. A 1984 US Bureau of Mines study found that HIP healed internal porosity in Ti-6Al-4V castings but did not significantly improve fatigue strength, and both cast conditions were well below wrought. Surface defects such as pin holes also matter. If the part is fatigue loaded, ask for fatigue data on your process.

Should alpha case come off by machining or by chemical milling?

Either can work, and the drawing or purchase specification should say which. Chemical milling in one lab trial took 30 to 40 minutes to clear the layer but removed more metal from thicker walls and raised hydrogen toward the 150 ppm limit cited from ASTM B367. Machining removes alpha case with the first cuts but hits the hard skin.

Need a quote for this part?

Send the drawing. We send one itemised quote for the finished parts and reply within 24 business hours.

Get a titanium quote

Keep reading