Home / Machining processes
Titanium Machining Processes
How titanium is milled, turned, drilled, threaded and EDM cut, what each grade asks of the tooling and coolant, and the tolerance and finish shops typically hold. Typical figures, never a promise. The shop that quotes confirms what it can hold on your geometry.
Why titanium needs its own process
Titanium is not especially hard. It is difficult because of where the heat goes and how the metal behaves at the edge. Ti-6Al-4V, Grade 5, is the grade most of this page is about, with Grade 2 noted where it differs. Every grade is on the grade reference.
- Heat stays at the edgeThermal conductivity around 7 W/m K for Ti-6Al-4V and 17 for Grade 2. The chip carries little heat away, so the tool edge runs hot and wears fast.
- Low modulusGrade 5 sits around 114 GPa, well below steel. Walls and long parts deflect under the cutter and spring back after it passes.
- Reactive and stickyAt cutting temperature titanium reacts with and welds to the tool. A rubbing edge builds up material, galls threads and hardens the surface it leaves.
- Fire hazard in finesChips, fines and grinding dust are flammable. Shops that cut titanium routinely manage swarf, coolant and extraction for it.
Process against part feature
Which operation makes which titanium feature, the tolerance it typically holds and what titanium changes in the setup.
| Process | Typical parts | Typical tolerance | What titanium changes |
|---|---|---|---|
| CNC milling, 3 axis | Brackets, plates, housings, manifolds | ±0.05 mm routine, ±0.02 mm with care | Low radial engagement and high axial depth. Trochoidal and adaptive toolpaths keep the edge cool. |
| CNC milling, 5 axis | Impellers, blisks, implant bodies, complex fittings | ±0.02 to ±0.05 mm on positions | Fewer setups, shorter tools and a constant tool angle. Often the cheaper route on complex titanium. |
| CNC turning | Shafts, hubs, fittings, valve parts | ±0.02 mm on fitted diameters, ±0.01 mm with care | Grade 2 makes long stringy chips. Chip breaker geometry and high pressure coolant control them. |
| Swiss type turning | Bone screws, dental implants, pins, small fasteners | ±0.01 mm on diameters is common | The guide bushing supports slender parts. Typical route for small medical parts in bar. |
| Drilling | Bolt holes, fluid passages, deep holes | Reamed or bored holes typically H7 | Through tool coolant and peck cycles. Drilling speeds sit well below milling speeds. |
| Threading | Fastener holes, fittings, implant threads | 6H and 6g classes typical | Galling risk on taps. Thread milling or form threads on external features at volume. |
| Wire and sinker EDM | Thin slots, sharp corners, hard to reach features | ±0.005 to ±0.01 mm typical on wire | No cutting force. Leaves a recast layer that fatigue critical parts usually need removed. |
| Grinding | Bearing journals, seal surfaces, tight flatness | Below ±0.01 mm on size | Specialist operation. Low stress grinding avoids surface damage and the dust is a fire risk. |
Starting cutting data by grade
Starting ranges for carbide from tool supplier titanium data. Every shop sets its own from its machines, tools and the part. Detail in titanium speeds and feeds.
| Operation | Grade 2 (CP) | Grade 5 (Ti-6Al-4V) |
|---|---|---|
| Milling, surface speed | around 60 to 100 m/min | around 30 to 60 m/min |
| Turning, surface speed | around 90 to 140 m/min | around 60 to 90 m/min |
| Drilling, surface speed | around 25 to 45 m/min | around 15 to 30 m/min |
| Feed per tooth, end mill | 0.05 to 0.15 mm | 0.05 to 0.12 mm |
| Radial depth, roughing | 30 to 50 percent of diameter | 10 to 25 percent of diameter |
Tooling and coolant
The decisions that separate a shop that cuts titanium every week from one that quotes it occasionally. More in titanium tooling and coolant and drilling titanium.
- SubstrateFine grain carbide, high cobalt for toughness. Titanium loads the edge heavily.
- CoatingAlTiN or TiAlN for roughing, which holds hardness at high edge temperature. Sharp uncoated or thin coated edges for finishing.
- GeometrySharp edge, positive rake, variable helix around 35 to 45 degrees against chatter, and a corner radius as large as the part allows.
- FeedA real chip load. A light, timid feed rubs, and rubbing is heat, galling and a hardened surface.
- CoolantHigh pressure through tool coolant where possible, flood emulsion otherwise. Aerospace and implant specifications often restrict chlorinated cutting fluids, so ask what the shop runs and how it cleans parts.
- WorkholdingRigid and short. Support thin walls, leave them until last and finish in light passes.
Thin walls, stress and heat treatment
Low modulus and trapped heat make thin titanium walls the fastest way to move a price. Up to about 5 to 1 height to thickness is routine. Above 10 to 1 the shop needs support material, staged removal and possibly a stress relief between roughing and finishing. See thin wall titanium parts.
Heat treatment in air grows an oxygen rich surface layer called alpha case. It is brittle and has to be removed by a finishing cut or chemical milling. If the part is heat treated after rough machining, leave stock for that. Welding and alpha case covers how shops check for it.
Tolerances and finishing
Routine is what shops quote without a conversation. With care adds time and inspection on every piece. Tighter needs a discussion before the drawing is signed. Detail in titanium machining tolerances and titanium surface finish.
| Feature | Routine | Achievable with care |
|---|---|---|
| General machined dimensions | ±0.05 mm | ±0.02 mm |
| Fitted diameters and bores | ±0.02 mm | ±0.01 mm |
| Position across faces, multi setup | ±0.08 mm | ±0.04 mm |
| Wall thickness, over 3 mm | ±0.1 mm | ±0.05 mm |
| Wall thickness, under 1.5 mm | ±0.15 mm | ±0.1 mm |
| Surface finish | Ra 1.6 µm | Ra 0.8 µm |
| Finish | Typical result | What it is for |
|---|---|---|
| As machined | Ra 1.6 to 3.2 µm | Most parts. Cheapest and often adequate. |
| Bead blast | Even matte, Ra 1.6 to 3.2 µm | Uniform grey appearance, hides light tool marks. |
| Passivation | Unchanged | Removes embedded iron and contamination. ASTM F86 is the usual reference for implants. |
| Electropolish | Ra 0.2 to 0.4 µm | Medical, vacuum and cleanliness critical parts. Removes material. |
| Anodize, AMS 2488 Type 2 | Unchanged | Matte grey. Wear resistance and anti galling. |
| Anodize, AMS 2488 Type 3 | Unchanged | Interference colours for colour coding and appearance. |
| Pickling or chemical milling | Depends on removal | Removes alpha case after heat treatment or hot work in air. |
Anodize colour is set by voltage and shifts with surface finish, so agree a sample when colour matters. See titanium anodizing.
Design for manufacture
Each line removes a decision a shop would otherwise make for you, and makes the quotes you get back comparable. Where the part ends up is covered by industry on the applications page.
- Name the grade and the standard, for example Ti-6Al-4V to ASTM B348 or AMS 4928
- Keep wall height to thickness under about 10 to 1, or expect support and staged removal in the price
- Give inside corners the largest radius the function allows
- Use ±0.02 mm or tighter only on fits, with ISO 2768-m on the rest
- Say whether EDM recast and alpha case must be removed, and how it is checked
- Put Ra only on the faces that need it and name the finish per surface
- State thread class and whether thread milling is acceptable
- Ask for a mill certificate to EN 10204 3.1 and lot traceability where the industry requires it
Process questions we get
Something not covered? Email .
Why is titanium slower to machine than steel?
Heat. Ti-6Al-4V conducts heat at around 7 W/m K against roughly 16 for 316L stainless and 167 for 6061 aluminium. The heat stays at the cutting edge instead of leaving with the chip, so shops run Grade 5 at around 30 to 60 m/min in milling, well below what the same machine runs in steel.
Does Grade 2 machine differently from Grade 5?
Yes. Grade 2 is softer and gummier, runs faster and is the easiest titanium to cut, but it smears if the tool is dull. Grade 5 is harder, roughly half the surface speed of Grade 2 and harder on tools. Most titanium quotes are for Grade 5.
Can titanium be wire EDM cut?
Yes. Titanium conducts, so wire and sinker EDM both work, and they suit thin slots, sharp inside corners and hard to reach features. EDM leaves a thin recast layer. On fatigue critical aerospace and implant parts, the specification usually requires that layer removed, so say on the drawing whether it applies.
Should titanium threads be tapped or thread milled?
Both are used. Titanium galls on a tap, and a broken tap in an expensive part is a scrap part, so many shops thread mill anything above small sizes. A broken thread mill usually costs a cutter rather than the part. Specify the thread class and let the shop choose the method.
Have a titanium drawing ready?
We own no machines. Send the drawing and we price it with partner shops that cut titanium and run the processes your part needs. You get one itemised quote. Reply within 24 business hours.