Fluorescent Penetrant Inspection of Titanium Parts: Process, Order and Callouts

Technician inspecting a metal part under UV light after fluorescent penetrant inspection

A crack in a machined titanium part can be too small to see and still large enough to end the part’s life under cyclic load. Fluorescent penetrant inspection, usually written FPI, is the standard way to find surface cracks before a part ships. It is cheap compared with most inspection methods, but it is easy to do badly, and on titanium the order of the process steps decides whether it finds anything. Many aerospace and some medical drawings call for it, and the callout often reaches the shop as a single line.

Diagram: FPI on Machined Titanium: Fluorescent Penetrant Inspection

This guide explains how FPI works, why titanium needs particular care, where the test sits in the process route and what to write on the drawing and RFQ.

What FPI is and what it finds

FPI uses a fluorescent liquid that seeps into surface-breaking flaws. After the excess is removed, a developer draws liquid back out of the flaw, and the flaw glows under ultraviolet light in a dark booth. An inspector reads the glow as an indication.

It finds flaws that are open to the surface: cracks, laps, seams, cold shuts and porosity that reach the surface. It does not find flaws below the surface or flaws that are closed. For internal flaws other methods apply, such as ultrasonic inspection of bar or forgings, which is why a mill certificate may carry its own test results for the raw stock. FPI does not measure flaw depth either. It shows where to look and how long the indication is.

The process steps

Shops follow a fixed sequence. The details come from the practice or customer specification in force.

  1. Pre-clean. The part is cleaned of oil, coolant and dirt, so penetrant can reach the flaw.
  2. Etch where required. A light acid etch removes smeared metal. See below.
  3. Dry. Moisture or solvent left in a crack blocks the penetrant.
  4. Apply penetrant. The part is coated or dipped, and the penetrant stays on for a set dwell time.
  5. Remove excess. Method decides how: a water wash, an emulsifier and then a wash, or a solvent wipe.
  6. Apply developer. A powder or liquid film that draws penetrant out of the flaw.
  7. Inspect. An inspector examines the part under ultraviolet light in a darkened area and records indications.
  8. Post-clean. All penetrant and developer are removed.

Method choice depends on the specification and the part. ASTM E1417 defines Type I fluorescent and Type II visible penetrants, and four removal methods.

Method Removal Typical use
A Water washable General production, rough surfaces
B Post-emulsifiable, lipophilic Higher sensitivity, finer cracks
C Solvent removable Local inspection, large parts, field work
D Post-emulsifiable, hydrophilic Higher sensitivity, controlled wash

Penetrant materials also come in sensitivity levels, from low to ultra-high. A higher level finds smaller flaws and also shows more background noise on rough surfaces. The drawing or specification sets the level when it matters.

Titanium-specific points

Etch before penetrant. Cutting, grinding and blasting can smear surface metal over small cracks. The cracks are still there, but closed at the surface, and penetrant cannot enter. Many aerospace specifications require an acid etch of machined titanium before FPI to open them. The shop’s etch step and its removal limits come from the specification. See titanium pickling and chemical milling for how etching removes metal and what it does to dimensions.

Low halogen and sulphur penetrant. Titanium is sensitive to certain contaminants. Penetrant standards require materials for titanium and nickel alloys to be controlled for halogen and sulphur content, so the shop uses materials that are certified for that use and keeps the certificates by lot. Ask whether the shop has done so.

Residues. Penetrant has to be removed completely after inspection. Residue on a part that later goes into heat treatment or welding can contaminate the surface. A careful shop post-cleans in the process route before any heat.

Inspect before peening, blasting or coating. Processes that deform the surface, such as shot peening or heavy blasting, can close cracks and hide them. Anodizing coats the surface and, again, can cover a flaw. FPI belongs before them. Titanium anodizing describes the coating step that follows.

Need a quote for this part? Get a titanium quote

Where FPI sits in the route

A typical sequence on a titanium part that needs penetrant inspection looks like this. The part’s own specification governs.

Step Why here
Rough machining Remove bulk
Stress relief Let the part move before finishing
Finish machining Bring to size, leaving allowance if an etch follows
Etch Open smeared surfaces, remove contamination
FPI Inspect while surface cracks are open
Post-clean Remove penetrant before any heat or coating
Anodizing or other finish After inspection, never before
Final dimensional inspection With the final surface

Because etching removes metal, dimensions are cut with allowance. A part that is machined to final size and then etched can drop below tolerance, so shops that do FPI often plan the allowance in advance. The effect on thin features is covered in thin wall titanium parts.

Who performs the inspection

FPI is an outside process in many shops. A specialist lab or an in-house NDT department performs it. The people who interpret indications are trained and qualified to a written practice, and aerospace customers often call for qualification to NAS 410 or a customer equivalent. Some customers also require the processor to hold NADCAP accreditation for non-destructive testing. Whether a given shop or lab holds it is a question to put to that shop, and the answer should name the scope. Ask for the specific accreditation or qualification and check it against what your drawing asks for.

On the shop side, ask which person signs the inspection report and what the report contains. A typical report names the part, the lot, the specification, the penetrant materials with lot numbers, the inspection date and the result.

Accept and reject criteria

The practice describes how to test. It does not decide what is acceptable. Acceptance criteria come from your drawing, your customer specification or the part’s design standard, and they usually list what is rejected outright, such as any crack or linear indication, and what is allowed in limited size or number, such as rounded indications.

Without a stated criterion, a shop cannot tell a defect from a harmless mark. Name the criterion on the drawing. Typical open questions to settle early are:

  • Is any linear indication a reject?
  • Are rounded indications allowed, and up to what size?
  • Do different zones of the part have different criteria?
  • What happens to a rejected part: rework and re-inspect, or scrap?

Rework such as light blending of a flaw is covered by the same specification and may need approval from the design authority.

Medical parts and consumer parts

Medical implants and instruments sometimes carry an FPI requirement, depending on the design. Titanium medical parts covers the standards and cleaning that follow. For aerospace work, titanium aerospace parts lists what an RFQ has to carry, and FPI is one of those items.

What to put on the RFQ

  • The FPI callout as written on the drawing: standard, type, method and sensitivity level.
  • The acceptance criterion and the zones, if they differ.
  • Whether etching before penetrant is required, and by which specification.
  • Personnel qualification and any accreditation the customer requires.
  • What inspection records and certificates must ship with the parts.
  • Where FPI sits relative to etching, peening, anodizing and final dimensional checks.
  • Whether the shop does FPI itself or uses an outside processor, and what that adds to the lead time.

Send the drawing with the inspection callouts on the RFQ form and shops reply within 24 business hours. If your drawing does not yet state a grade, the titanium grades reference can help you pick one.

See also: the titanium aerospace parts reference.

Frequently asked questions

What does fluorescent penetrant inspection find in titanium?

It finds cracks, laps, seams and porosity that break the surface. It does not find flaws below the surface, which need ultrasonic or other methods. The test works only if the defect is open to the surface when the penetrant goes on.

Why is titanium etched before FPI?

Machining can smear surface metal over small cracks and close them, so penetrant cannot enter. A light acid etch or other approved metal removal opens the surface. Many aerospace specifications require this step on machined titanium before penetrant inspection.

Which standards cover FPI on titanium?

ASTM E1417 is the common practice for liquid penetrant testing and AMS 2644 covers the inspection materials. NAS 410 sets personnel qualification for many aerospace customers. Your drawing or purchase order names which apply, and a shop will state which it works to.

Need a quote for this part?

Send the drawing. We send one itemised quote for the finished parts and reply within 24 business hours.

Get a titanium quote

Keep reading